Some facts and hypotheses related to thermal analysis with ATAS.
Author: Rudolf Sillén
Technical Director, NovaCast AB
Shrinkages are one of the most common casting defects. The main cause of shrinkage cavities is the fact that all commercial alloys contract when a casting cools from the pouring temperature to solidus. The contraction is usually between 1-5 % depending on the type of alloy and the pouring temperature. The main contraction occurs between the pouring temperature and the liquidus temperature. If the contraction is not compensated for by feed metal, either by supplying feed metal or by forming a depression of the outer surface, a shrinkage cavity will occur. Cast iron alloys, which solidify with a precipitation of graphite, represent a more complex behavior, the reason being
that the dissolved carbon partly precipitates as graphite with a lower density than the base iron. The precipitation is therefore associated with an increase in volume, which in some cases partly might offset the contraction of the liquid and the austenite.
In the following we have classified shrinkages in four basic types. We will discuss how they occur and how they can be avoided. The four basic types are Outer sunks (pull downs), Macro shrinkages, Micro shrinkages and Porosities.
A. Outer Sunks
A1 - Definition and location
Outer sunks (pull downs, sinks) can be seen from the outside of the casting, usually as a smooth depression in the casting surface. They are normally located on thick sections of the casting and on surfaces located on the top of the casting during pouring. Outer sunks are also referred to as "pull downs" and they can occur not only on horizontal top faces of the casting but sometimes also on vertical surfaces.
A2 - The basic mechanism behind outer sunks
The metal starts to solidify at the surfaces of the mould cavity and a thin skin is formed. The temperature drops further, which causes the liquid and the semi-liquid metal inside the casting cavity to contract further. If no feed metal is available either from the gating system or from a feeder then contraction will cause a negative pressure inside the cavity. In order to equalize the pressure difference between the atmosphere and the interior the solid outer skin will be "pulled" inwards. The effect is that the contraction is compensated for by a reduction of the volume of the casting. Thus outer sunks develop at an early stage of the solidification process
before the massive eutectic freezing has commenced.
A3 - Variables that influence the creation of outer sunks
The major variables that influence the likelihood for development of outer sunks and their effect are as follows:
- Too high pouring temperature. The volumetric contraction is about 1.4% per 100 C for cast iron. Thus an increase in pouring temperature of 50 C will increase the need for feed metal with 0.7%. When pouring castings with small modulus in ductile iron, a higher pouring temperature might decrease shrinkage tendency especially in hard moulds. The reason is a better temperature distribution in the mould and less fast initial cooling.
- Insufficient amount of feed metal available at early stages of the solidification. Normally no feeder is needed for castings with small modulus (less than 0.4 cm). Feed metal can be supplied from the pouring cup through the gating system. However, if the modulus of the ingate is too small then feed metal might be lacking.
- Deformation (expansion) of the casting cavity. This might happen in green sand moulds and cause mould wall movement, which increases the casting cavity.
- Too high liquidus temperature. A liquidus temperature higher than what the system has been designed for will cause the surface skin to form earlier and thereby increase the risk for outer sunks.
- Too high amount of primary austenite (S1) cause by too low active carbon equivalent. A higher amount of primary austenite than usual for the alloy means that the contraction increases at an early stage.
- Too low eutectic minimum temperature (TElow). A eutectic temperature that is lower than the normal minimum level means that the contraction of austenite is higher than normal as the distance between liquidus (TL) and the eutectic temperature (TElow) increases. Iron undercooling below the graphitic eutectic due to lack of nucleation - too little or wrong type of inoculation or faded inoculation.
- A solidification that favors skin freezing (Also see number 5).
- Insufficient weighting or clamping of the mould. This might have the same effect as a deformable mould especially if the casting has some parts with lower modulus than solidify quickly and cause a pressure that tends to separate the mould halves.
- Riser does not pipe due to too low height, too low modulus or too large modulus of the ingates.
A4 - Which variables can be monitored by ATAS?
Thermal analysis can be used to monitor the metallurgical variables that influence the development of outer sunks. ATAS is especially designed to monitor and interpret cooling curve data and to predict the potential risk for shrinkages and also other problems. The metallurgical variables used to predict outer sunks are liquidus (TL), liquidus plateau, primary austenite (S1) and the low eutectic temperature (TElow). (Parameters number 4,5,6 and 7). The illustration shows a typical cooling curve for a hypoeutectic iron and the "time-position" for various types of shrinkages.
ATAS makes it possible to monitor and control these metallurgical variables. However, as can be understood from chapter A3, several other variables do influence the outcome. Even if the metallurgical variables are within their acceptable limits outer sunks might occur, e.g. if the pouring temperature is higher than normal or the mould is softer. Also the reverse might be true - the metallurgical variables might be slightly outside their normal limits but no shrinkage will occur because the mould was much harder than normal or the pouring temperature was lower than normal.
The important fact is that ATAS allows the foundry man to ensure that 4 out of 8 variables are within the specification.
A5 - How can out sunks (pull downs) be avoided?
The pouring temperature must be chosen individually for the casting - e.g. castings with small modulus and/or long flow length must use a high pouring temperature and/or be poured very fast to avoid casting defects such as cold shuts. Castings with a high modulus and/or short flow length can be poured with a low temperature. To minimize the volume contraction in liquid state, the general advice is to use as low a pouring temperature as possible without getting any casting defect. The feeding system can be designed and dimensioned once the optimal pouring temperature has been established for a casting. Mould hardness must also be considered when dimensioning the feeding
system. It should be as high as possible.
Feeding from the gating system is normally sufficient if the casting modulus is less than 0.3 cm. However, make sure that the ingates do not freeze off too early and thereby block the flow of feed metal from the pouring cup.
In some cases where a casting has been successfully made without a feeder, that is using ingate feeding, shrinkage occurs when a ceramic filter is placed in the gating system. A filter reduces the modulus locally and might block the feeding path.
If the modulus is larger than 0.3 cm then it is recommended to use a feeder. A feeder, which only has the purpose to eliminate outer sunks, can be made smaller than if it also has to assist in eliminating macro shrinkages (as they are developed at a later stage).
From a metallurgical standpoint the main thing is to reduce variations in the process variables TL, S1 and TElow. If ATAS is used to monitor these variables it will soon become evident how to melt, hold and treat the metal to reduce variations.
B. Macro shrinkages
B1 - Definition and location
Macro shrinkages are usually found inside the casting and close to heat centers. They appear as larger holes, usually with rough surfaces, often dendritic and are often larger than 5 mm. Macro shrinkages are usually not revealed unless the casting is machined or deliberately cut through sections of heat centers. Can also appear in or close to ingates.
B2 - The basic mechanism behind macro shrinkages
Macro shrinkages develop after the initial solidification on the surface when a shell that can not be deformed by the pressure difference to the atmosphere. If no more feed metal is available at that point in time then the contraction of the liquid and semi liquid metal as well as the already solidified parts results in a cavity.
B3 - Variables that influence the creation of macro shrinkages
Shrinkages are influenced by the behaviour of both the alloy and the mould. The dominating variables for macro shrinkages are:
1. Insufficient supply of feed metal - too small feeder modulus or feeder neck or feeder does not pipe due to too large ingate modulus or height position.
2. Feeding path closed too early - wrong position of feeder. More dendrites than usual at an early stage (CLF factor in NovaSolid). Too low active carbon equivalent (ACEL=the true carbon equivalent measured with ATAS). For ductile iron, ACEL should be eutectic and carbon minimum 3.6%.
3. Mould hardness during solidification. Soft moulds which favor mould wall movement. A green sand mould, hard at room temp can be soft during solidification due to the high water level in the condensation zone.
4. Mould weighting or clamping insufficient to stand the pressure during solidification. Eutectic pressures up 50 kg/cm2 has been claimed!
5. Higher liquidus temperature (TL) than normal. In hypoeutectic irons this means too much primary austenite and more difficult feeding. In hypereutectic it means more primary graphite which reduces the amount of eutectic graphite.
6. Higher amount of primary austenite (S1) than normal. Too low ACEL.
7. Too high recalescence and recalescence rate causes expansion from graphite to occur too early. (In ductile - too much late inoculation with low ACEL).
8. Too low eutectic temperature might cause some primary carbides to form.
B4 - Which variables can be monitored by ATAS?
ATAS can monitor variables 5,6 and 8. The length of the liquidus plateau can also be used to indicate anomalies in the initial dendrite growth and precipitation of a pro-eutectic phase.
B5 - How can macro shrinkages be avoided?
The remedies are basically the same as for outer sunks. However to avoid macro shrinkages the feed metal must be available longer than for Outer sunks because macro defects occur at a later stage during solidification. A solidification simulation e.g. using NovaSolid is highly recommended to ensure that feed metal can reach critical areas and that feed metal is available during the contraction period.
C. Micro shrinkages
C1 - Definition and location
Micro shrinkages are smaller cavities with irregular surfaces often with signs of dendrites. Sizes are often less than 3 mm. The defects are usually located close to heat centres in the casting. Micro shrinkages are often referred to as porosity or "leakage" as castings with this type of defect often leak during a pressure test. Micro shrinkages are usually not revealed unless the casting is machined or deliberately broken.
C2 - The basic mechanisms behind micro shrinkages
The defects occur at the latest stages of solidification. It is therefore more difficult to solve micro shrinkage problems by changing the gating or feeding system. Micro shrinkages are more of a metallurgical problem. There are three basic mechanisms behind micro shrinkages.
The first and most common mechanism behind micro shrinkages is that the contraction of the austenite (primary and eutectic) at the end of freezing can not be compensated for by the precipitation of carbon into graphite, which is associated with an increase in volume. (The density of the austenite is approximately 6.9 g/cm3 at temperatures around 1100 and the density of graphite about 2.3 g/cm3).
Another reason especially in gray iron is too high levels of nitrogen. In ductile iron this is less likely as the high CEL-level reduces solubility of nitrogen. High nitrogen levels cause an increased solubility of hydrogen. During the end of solidification a dispersed type of shrinkage usually occurs in almost all of the casting. The cavities look like a "comma" and are often referred to as "comma" cavities or sometimes comma gas blows. Adding about 0.02% titanium usually helps. Another alternative is to use zirconium especially with ductile iron.
The other mechanism is that due to the composition of the iron there are one or more phases that solidify at a lower temperature than the austenite-graphite eutectic. The most well-known case is the formation of iron phosphide (Fe3P) in gray iron if the phosphorus level is higher than 0.15 %. The Fe3P phase segregates to cell boundaries where it continues to contract even after most of the alloy has solidified. The solidus temperature for Fe3P is about 850 C.
C3 - Variables that influence the creation of micro shrinkages
- Mould stability. Too soft moulds, which might cause mould wall movement.
- Too little sea coal addition to green sand.
- Bentonite (Calcium) with low wet compression strength in green sand. Sodium bentonites are optimal for reducing shrinkages.
- Insufficient weighting or clamping of moulds.
- Too little eutectic graphite especially at the end of freezing; its precipitation can not compensate for the shrinkage of the austenite. A true eutectic composition with relatively high silicon level is preferred as the amount of eutectic graphite is maximized. (Note that the eutectic point is a function of the thermal modulus!).
- Too much inoculant in gray iron that reduces cell size.
- Too high hypereutectic composition in ductile iron. If too high then some of the dissolved carbon will be precipitated as primary graphite and the amount of eutectic graphite might be insufficient. Evidenced by too many large size nodules which have been growing early in the liquid.
- Too high phosphorous in gray iron - max 0.12 % and max 0.03% if molybdenum or high chromium levels are used in the alloy.
- Too much magnesium in ductile iron. Levels of Mg and RE must be consistent with the thermal modulus of the casting.
- Too high amount of phases which exhibit solidus below 1100 C. e.g. Fe3P.
- Too high recalescence and recalescence rate causes expansion too early.
- Too low eutectic temperature might cause some primary carbides to form.
- Too small Graphite Factor 1 (GRF1) indicating too small amount of eutectic graphite during the second part of the eutectic.
- Too high Graphite Factor 2 (GRF2) indicating too little eutectic graphite precipitation at the end of freezing.
- Too low solidus (TS) which may induce carbides at the last portions to freeze. Too high levels of Mg, Nb, V or similar elements tend to segregate to the grain boundaries and form carbides that contract during their solidification. For normal ductile iron TS should be above 1100 C.
- Too high silicon will increase segregation of carbide forming elements, which increases the tendency for micro shrinkage.
C4 - Which variables can be monitored by ATAS?
The mechanism behind micro shrinkages is dependent on the metallurgical status of the melt, which can not be measured by chemical analysis. The ATAS thermal analysis method is therefore a powerful tool for measuring and verifying that a melt is within acceptable metallurgical threshold values. ATAS can also be used to study the result of changes in melting and treatment variables and alloying materials, whereby the most optimal alloying materials as well as melting and treatment processes can be established. ATAS factors 10, 11, 12,13 and14 as mentioned in the previous chapter are good indicators for micro shrinkages.
C5 - How can micro shrinkages be avoided?
The first condition is to have a hard mould - ideally chemically bonded sand moulds. A green sand mould is compressible, however hard at room temperature, because of the formation of a condensation zone. In the condensation zone, which travels from the surface of the cavity and inwards, the moisture content can be up to 3 times higher than the initial value. This means that the bentonite layer becomes semi-fluid and can easily be compressed. However green sand moulds can be made more stable by means of the following recommendations:
- A sodium bentonite is most favorable, as its wet compression strength is high.
- Use sea coal as carbon additive. It will "coke" and increase the friction between sand grains. The carbon level in the sand should be at least 5 %.
- Use as low moisture as possible. The compactability should be less than 40%.
- The moulding machine should be able to compact the sand properly.
- On Disamatics check that the mould conveyor is working properly so that the moulds are kept together tightly (sometimes a gap can be formed).
- For larger flasks use flasks with bars - make sure the moulds are clamped properly or that enough weights are put on the cope.
- The forces during solidification of cast iron can be very high - therefore normal weighting to avoid run-out at the parting line is not enough.
Metallurgically, the most important factor is to ensure that a sufficient amount of carbon is precipitated as graphite during solidification. It is important that the initial growth rate is not too high. This can be indicated by studying the recalescence and recalescence rate on ATAS. A too high rate means too much graphite too early, which is associated with an expansion that can cause mould wall movement and thus increase the likelihood for shrinkages. Base iron nucleation status is important. Super heating above approximately 1520 C too long reduces the nucleation level. (ATAS users can easily make some tests with some melt to find the exact limits valid with their
iron composition (equilibrium temperature), type of furnace (surface area, stirring action), etc).
Graphite factor 1 indicates the precipitation of graphite during the second phase. Higher values are more favorable. However this factor requires that the Quik-Cup always be filled to the brim, otherwise the weight of the samples is different, which will influence this factor.
It is essential that enough graphite be precipitated at the end of freezing. Studying graphite factor 2, the first derivative at solidus and the solidus temperature can indicate this. A low graphite factor 2 is favorable. The first derivative (dT/dt_TS) should be as low (deep) as possible. Solidus should be high to ensure that the last metal solidifies gray and not as partly white (which does not expand).
These metallurgical factors can be influenced by selection of charge materials, charging sequence, the melting cycle (temp/time steps) as well as type and amount of alloying materials, inoculants and FeSiMg. With ATAS it is possible to find the optimal melting and treatment practice to reduce the likelihood for shrinkages. Such an optimization can NOT be made using traditional chemical analysis alone. The behavior of a melt depends not only on the percentage of each element but also on formed compounds such as oxides, silicates, sulphides, nitrates and their interaction during solidification. The total behavior can however be revealed by means of ATAS thermal analysis. A
quantitative analysis of the solidification can also be made which allows the user to study the precipitation of graphite and the associated volume changes in details. ATAS shows the weight of precipitated graphite during the different phases of solidification as well as the need for feed metal.
Metallurgically it is also important to avoid phases that have a solidus temperature below the main solidus temperature. In gray iron the phosphorous level should normally be less than 0.12 %. If molybdenum or chromium are present then the phosphorus level must be lower - in some cases less than 0.4% to avoid porosity. In ductile iron phosphorous should be less than 0.03%.
D. Porosities
C1 - Definition and location
Porosities are small, dispersed cavities with irregular or rather smooth surfaces, often less than 1 mm in size. The defects are usually located close to heat centers and in grain boundaries. They are more dispersed than micro shrinkages. Typically, the defect is not discovered until the casting is subjected to a leakage test with water or air.
C2 - The basic mechanism behind porosities
The defects occur at the very latest stages of solidification. Therefore it is not possible to solve porosity problems with changes in the gating or feeding system (unless a very steep temperature gradient is maintained). Porosities are a metallurgical problem mainly depending on the chemical composition.
The main mechanism is that due to the composition of the iron, one or more phases solidify at a lower temperature than the austenite-graphite eutectic. The most well-known case is the formation of iron phosphide (Fe3P) in gray iron if the phosphorus level is higher than 0.15 %. The Fe3P phase segregates to cell boundaries where it continues to contract even after most of the alloy has solidified. The solidus temperature for Fe3P is about 850 C. The problem is aggravated by Mo and Cr. Another cause can be that the iron has too high levels of elements like Nb and V that usually originate from steel and segregate to the grain boundaries and form carbides.
In ductile iron too high magnesium levels can cause similar problems as magnesium segregates to the rest melt and can induce formation of carbides which contracts and creates porosity.
C3 - Variables that influence the creation of porosities
- Too high phosphorous in gray iron - max 0.12 % and max 0.03% if molybdenum or high chromium levels are used in the alloy.
- Too much magnesium in ductile iron.
- Too high amount of phases which exhibits solidus below 1100 C. E.g. Fe3P.
- Too high levels of Nb, V etc.
C4 - Which variables can be monitored by ATAS?
As the mechanism behind porosities is more dependent on solidification of minute phases with a temperature below the normal solidus it is normally not detectable by thermal analysis. Some guidance might be available by studying TS and the last part of the first derivative curve.
C5 - How can porosities be avoided?
The phosphorous content should be less than 0.12 % in unalloyed gray iron. (But minimum 0.08% in order to avoid expansion penetration!). The gas content can also influence this type of defect. Metallurgically it is important to avoid all phases, which have a solidus temperature below the main solidus temperature. In gray iron the phosphorous level should normally be less than 0.12 %. If molybdenum or chromium is present then the phosphorous level must be lower - in some cases less than 0.04% to avoid porosity (leakage). The amount of magnesium in ductile should be kept to a minimum.
E. "Riserless" methodology
Many castings are successfully produced without a riser (i.e. a feeder). Basically there are four possibilities:
- The customer accepts some shrinkages as their influence on the functionality of the casting is negligible, e.g. a counterweight can be allowed to have inner shrinkages. Many micro shrinkage defects influence neither the strength of the part nor the appearance - however the foundry often takes for granted that the customer expects a completely sound casting. Usable castings are often scrapped without any rational reason! A dialogue between the foundry and the customer based on solidification simulations before start of production can often result in more realistic quality demands, which will benefit both parties (higher yield, less problems!).
- The modulus of the casting is fairly small (less than 0.3 cm) and the pouring time is relatively short. In this case the feed metal is taken from the pouring cup as long as feeding is possible through the ingates. Note that the modulus, i.e. the solidification time of the gating system, must be related to the modulus of the casting in order to allow feeding. A simulation e.g. with NovaSolid is ideal to find the optimal design.
- The modulus of the casting is fairly small and a main part of the casting geometry is like a thin plate. In such cases the initially solidified thin skin is depressed inwards by the atmospheric pressure. The depression might only be fractions of a millimeter but on a larger surface this will add up to a large volume, which will compensate for the shrinkage.
- The alloy (ductile) should be close to true eutectic composition which is related to the cooling rate. That means that the liquidus temperature is very low (around 1145-1150) and the solidification starts with the precipitation of eutectic (graphite and austenite). Thus the contraction of pro-eutectic austenite is eliminated. A hyper-eutectic solidification in the casting should be avoided as it will reduce the amount of carbon during the eutectic reaction. (Note that the chemical composition can be hyper-eutectic but the solidification hypo-eutectic if the cooling rate is high). The pouring temperature must be very low in order to reduce the contraction of the melt in
liquid state. Pouring temperatures for "riserless" castings are preferably around 1200 C. Due to the low pouring temperature, the pouring time must be short, to avoid defects. Two other conditions must also be fulfilled. First the modulus of the casting must be at least 1.5 cm. This will ensure that the solidification time is slow enough to allow the eutectic reaction to occur slowly in order to precipitate as much eutectic graphite as possible. In order to avoid mould wall movement due to the forces during solidification the moulds must have sufficient strength. Chemically bonded moulds using binders such as furan or cement must be used. The moulds should be
firmly clamped (instead of using weights).
Illustrations from ATAS Screens:

Pic. 1. The cooling curve shows a eutectic ductile iron with a high recalescence.

Pic. 2. The same cooling curve evaluated by ATAS. Several parameters are outside the allowed thermal limits. The expert system gives a warning that this iron is prone to micro shrinkage defects. Pressing the Risk&Explain icon will give further information.

Pic. 3. This screen shows how the expert system has interpreted the thermal data.

Pic. 4. The cooling curve has been analyzed quantitatively by ATAS. In total 7.3 grams of graphite has been precipitated. Some of it has been precipitated just before the eutectic temperature (at the walls of the Quik-Cup). The problem is that too much is precipitated too early (Eutectic 1=32.7%). The solution is to improve the treatment and inoculation process. As the effect of various modifications now can be visualized and quantified it is easy to optimize the various processes.
Version 02-07-22.
|